Most enquiries reduce galvanizing to one line: hot dip galvanized to EN ISO 1461. That line settles the coating and almost nothing else. Whether a closed box section can be coated on the inside, whether a frame still fits its mating part after a dip in molten zinc at around 450 °C, and whether a tapped hole still takes a bolt are all decided by details on the fabrication drawing. Those details are cheap to add at enquiry stage and expensive to discover at inspection.

The process is easy to describe. Prepared steel is immersed in molten zinc and the zinc reacts with the surface to form a bonded coating. ISO 1461:2022 specifies the coating properties and the test methods for articles galvanized after fabrication. What the standard does not do is design the part for you.

What the bath allows you to build

A galvanizing kettle is a fixed box of molten metal. Anything longer, taller or wider than the usable working volume has to be immersed twice, from opposite ends, and the overlap zone gets a visible mark where the two passes meet. That is a normal outcome for long beams, but it has to be agreed before the drawing is released, because the overlap area also tends to hold a heavier coating.

Weight and lifting matter as much as size. The part is picked up, dipped, withdrawn and quenched, so the fabricator needs lifting points that survive the bath and do not collect zinc. On a large frame this is a rigging plan, and it is worth asking who writes it.

Vent and drain holes decide whether the inside gets coated

Every enclosed volume needs an opening at its highest point and one at its lowest point, in the orientation the part will actually be dipped. Air leaves through the top, zinc enters and leaves through the bottom, and no internal baffle may block the path between them. ISO 14713-2:2019 is the design guidance for this, and it exists because a sealed cavity dipped in molten zinc can eject metal.

Three things belong on the drawing rather than in a covering note:

  • The holes must be on the drawing with a position and a size. If they are missing, the fabricator either adds them where convenient or leaves them out, and you find out at inspection.
  • The size depends on the cavity and on the galvanizer's practice. It is agreed with the galvanizer, not copied from a previous job.
  • A hole that is drilled after fabrication can land in a plate that is already machined or a face that is already prepared.

On a machinery frame the usual offenders are box-section outriggers, closed stiffener pockets, tubular guards and hollow gussets. A short list of these parts, agreed at enquiry, removes most of the risk.

Distortion shows up after the dip, not before

Welding already leaves residual stress in a frame. A dip at around 450 °C relaxes part of it, and a frame that was straight on the bench can come out with a bowed flange or a twisted end. Asymmetric sections are the classic case: a heavy plate welded to thin sheet, or a channel stiffened on one side only.

The answer is a fabrication sequence that balances weld heat and a straightening step before galvanizing. Straightening after the coating is applied damages the zinc, and repair coatings do not restore the original performance. A frame with machined pads or a flat mounting face needs that face called out on the drawing: either it is machined after galvanizing, or flatness is measured after the dip. Both requirements cannot be met without an agreed allowance.

Threads, fits and machined registers

A zinc coating builds on every exposed surface. EN ISO 1461 sets minimum thickness by steel thickness, and for plate over 6 mm the figures are 85 µm mean and 70 µm local. A tapped M12 hole with a normal tolerance will not accept a bolt after that.

The options are standard and each one has a cost:

Approach What it means on the drawing
Over-tap the thread Thread cut oversize to leave room for the coating, called out per hole
Mask or plug Coating suppressed on the thread, usually with a plug or a lacquer
Machine after coating Thread or register cut after galvanizing, coating opened at the edge
Galvanized fastener Standard fastener coated to its own specification, such as EN ISO 10684

The same logic applies to dowel holes, bearing seats and close-clearance spigots. A machined register that carries a bearing cannot receive a 70 µm coating and stay in tolerance, so either the register is masked or it is machined afterwards. Buyers who list the masked faces in the RFQ get a price that includes the masking. Buyers who do not get a frame with the coating ground off the register and a conversation about who pays for it.

Trapped pickle weeps for months

Two plates clamped or welded with a gap between them behave like a capillary. Acid from pickling and flux residues enter the gap and come out later as a stain or a corrosion site, often after the frame has been painted or shipped. Continuous seal welding around the gap closes it. Where that is impractical, the overlap is a known weak point and should be recorded as such.

What the standard asks you to accept

EN ISO 1461 is written in terms of minimum coating thickness, measured on the article, with a local value that no single reference area may fall below and a mean value for the article. For steel over 6 mm the requirement is 70 µm local and 85 µm mean; between 3 mm and 6 mm it is 55 µm and 70 µm; between 1.5 mm and 3 mm it is 45 µm and 55 µm. Thinner material drops again.

A thicker coating cannot simply be bought by asking for one. Coating growth depends on steel chemistry and immersion time, and a very thick coating can be more brittle. If a project asks for a heavier coating than the minimum, the conversation with the galvanizer happens before the quotation, not after. A certificate of conformity with recorded thickness readings is the normal evidence, and it belongs in the RFQ as a deliverable rather than as a favour at the end of the job.

Steel chemistry changes the finish

Silicon and phosphorus in the steel affect how the zinc layer grows. Reactive steel produces a thicker, darker and sometimes uneven coating. That is within the standard, and it is the reason two frames from the same drawing can look different. If the frame will be visible, state which faces matter and what "acceptable" means, and expect colour variation across heats. Writing "uniform light grey finish" into an RFQ that also cites EN ISO 1461 creates a requirement the standard does not support.

Repair, site welds and the end of the coating

Galvanized frames are often modified on site: a bracket added, a hole enlarged, a guard re-drilled. Each of those operations opens the coating. Zinc-rich repair paint is the usual remedy and it is not equivalent to the original coating, so decide in the contract who is allowed to modify the frame, who repairs it and what evidence is required.

The same question applies to transport damage. A frame that arrives with a scuffed corner is a commercial issue unless the acceptance rule was agreed in advance.

What belongs in the contract manufacturing RFQ

A galvanizing clause that can be quoted without assumptions carries the following:

  1. The standard and edition, and whether the coating is a minimum or a specified thickness.
  2. Who owns vent and drain hole design, and who approves the positions.
  3. The list of masked faces, threads and registers, with the method for each.
  4. Flatness and fit requirements that apply after galvanizing, not before.
  5. Lifting points and the lifting plan for oversize parts.
  6. Appearance acceptance for visible faces.
  7. Thickness records and a certificate of conformity.
  8. Repair responsibility and the method allowed.

Each item changes either the price or the delivery risk, which is why a quote that omits them is not comparable with one that includes them. If paint is also in scope, the two finishes need separate clauses rather than one sentence about surface treatment.

Where responsibility sits

The designer or buyer owns the coating class, the drawing details that make coating possible and the acceptance criteria. The fabricator owns execution: hole positions if the drawing is silent, weld sequence, dimensional result and the record of what was measured. The galvanizer owns the coating to the standard it was given. On a frame supplied by Realjet, the part is fabricated to your drawing and galvanizing is arranged as a process step within the quoted scope, with the scope itself confirmed in the quotation.

Before the enquiry goes out, the useful test is simple: could a fabricator quote the galvanizing without asking a single question about holes, threads or flatness? If not, the missing answers are the ones to write down. The contract manufacturing capability page sets out how fabricated frames and machined interfaces are handled, and the guide to surface treatment and coating scope covers the paint side of the same decision. For frames where heat has already moved the geometry, welding distortion control explains what can be corrected before the dip.